Weld Lines in Injection Molding: Knit Line Causes and Fixes

Last Updated: October 24, 2026

Answer Capsule: A weld line in injection molding is the seam where two melt fronts meet and fuse, usually behind a hole, boss or core pin. The seam can hold 20 to 100 percent of the resin’s strength, and glass-filled resins land at the low end. Fixes run from fill speed and venting to moving the gate.

A faint line runs across your housing right where the melt split around a screw hole. The part cracks there in drop testing. That line is a weld line in injection molding, also called a knit line.

On a show surface it is a cosmetic reject. On a snap fit it is a field failure. Weld lines are the one defect you cannot fully process away. Every hole, boss, core pin and second gate splits the flow, and the fronts must meet somewhere.

This post covers how to tell a weld line from a flow line, why the seam is weak, and the fixes in the order a molder tries them. It ends with the design rules that put the seam where it does no harm. The numbers come from Plastics Technology. The fix order is how Brent Hanke works a weld line problem at Legacy Molding in Phoenix.

What does a weld line look like, and how is it different from a flow line?

A weld line is a thin, straight seam on the surface. It always sits downstream of something that split the flow: a hole, a boss, a core pin or a second gate. Flow lines are different. They are wavy ripples that follow the flow front near the gate or at a wall change.

Two quick tells. A weld line often catches a fingernail as a tiny notch, while a flow line feels smooth. A weld line runs away from the obstacle, and a flow line wraps around the gate.

What causes weld lines in injection molding?

Weld lines form when the melt splits around an obstacle and the two fronts meet with a cool, stiff skin that does not fully mix. Two things decide how well the seam heals: whether the polymer chains tangle across the boundary, and whether trapped air holds the fronts apart. John Bozzelli, writing in Plastics Technology, puts both ahead of melt temperature as the real root causes.

The causes sort into the four buckets Legacy Molding uses on every defect review.

Bucket What causes or worsens the weld line
Material Glass or mineral fill, semi-crystalline resins, stiff grades, effect pigments, excess mold release
Process Slow fill, low melt or mold temperature, early switch to hold, low pack pressure
Tool No vent at the meeting point, unvented blind holes and ribs, small gate, fronts meeting head-on at a load point
Design Holes and bosses in the flow path, wall changes that race one front ahead, a second gate on a cosmetic face

How much strength does a weld line cost?

A weld line can leave the part with about 20 percent to nearly 100 percent of the resin’s nominal strength, according to Bozzelli’s guide. In his test data, neat polypropylene kept close to 90 percent of its strength across a weld. The same polypropylene with 30 percent glass kept only 34 percent. The fibers line up with the flow and cannot cross the seam.

On your drawing: a weld line on a non-load face of unfilled ABS or polycarbonate is usually fine. On a glass-filled nylon snap fit it is the weakest point in the part, and the gate has to move it.

How do you fix weld lines, in order?

Start with process, because it is free. Then venting, because it is cheap. Then the gate, because it costs steel.

  1. Fill faster. Higher injection velocity gets the fronts to the seam hotter. Form the weld during first-stage fill, not during pack.
  2. Raise melt and mold temperature inside the resin maker’s window. Bozzelli suggests about 10 degrees C on the mold as a sensible step.
  3. Switch to hold later and pack harder, so the seam is pressed to the steel while it is soft.
  4. Vent the meeting point with a parting-line vent, a vented core pin or a porous steel insert. Bozzelli calls venting the one tooling issue not to compromise.
  5. Add an overflow well. A small dummy cavity past the seam pulls melt through the weld after it forms. A 2022 Plastics Technology study on a glass-filled part cut the modulus loss at the weld from about 35 percent to about 16 percent.
  6. Move the gate so the fronts meet in a low-stress, hidden area with some flow after the seam.

Design rules that keep weld lines out of trouble

Here is a call Legacy Molding gets most months. An engineer has a polycarbonate bezel with four mounting holes along the top edge and a clear window below. Every sample shows four faint lines running from the holes into the window. Process changes faded them but never cleared them.

The holes sat between the gate and the window, so the seams had to land in the window. The fix was in CAD. Gate from the bottom edge so the window fills first, and let the holes split the flow at the end of fill where nobody looks.

Rules that prevent that call:

  • Gate so holes and bosses are the last thing the melt reaches, or sit off the main flow.
  • Keep walls uniform. Bozzelli’s limit is 25 percent variation for amorphous resins and 15 percent for semi-crystalline resins.
  • Run ribs along the flow, and put the seam in a corner or on a non-load face.
  • Pick the resin with the weld in mind. A glass-filled part that needs strength at a hole may need a thicker local section or a metal insert.

Legacy Molding’s DFM review flags every hole and boss in the flow path before a tool is cut. The injection molding design guide covers the wall, rib and gate rules. The injection molding defects hub shows how weld lines relate to the other nine common defects.

When does a weld line need a tool change?

A weld line needs a tool change when process limits are used up and the seam still fails on strength or still shows on a visible face. The signs: it breaks in a pull or drop test at every setting in the resin’s window, it sits in the middle of a cosmetic face, or it burns when you fill faster because the vent is missing. Venting is often done in a day. A gate move or an overflow well is a steel change through the tool shop, followed by a fresh first article.

What to ask your molder about a weld line

Ask where the seams are, what they held in testing, and what changed between the good lot and the bad lot. A corrective-action note should state the cavity and seam location with a photo, the settings before and after (injection velocity, melt and mold temperature, switch-over point, pack pressure and time), the vent condition at the seam, and the test result with the setup sheet revision. Brent Hanke keeps the setup sheet and the FAI together on every Legacy Molding tool, so the fix is recorded, not remembered.

Frequently Asked Questions

Are weld lines and knit lines the same thing?

Yes. Both names describe the seam where two melt fronts meet. A meld line is a seam formed at a shallow angle, usually stronger and less visible.

Can weld lines in injection molding be eliminated completely?

Not on a part with holes, bosses or more than one gate. The seam can be moved, strengthened and made nearly invisible, but any obstacle in the flow creates one.

Do weld lines weaken a molded part?

Usually. Strength at a weld runs from about 20 percent of nominal to close to 100 percent. Unfilled amorphous resins lose the least and glass-filled resins lose the most.

Does raising mold temperature fix weld lines in injection molding?

It improves the look and sometimes the strength, but it does not remove the cause. Venting and gate location are the lasting fixes.

Conclusion

Weld lines form wherever the melt splits and rejoins. Process gets you the appearance, venting and gate location get you the strength, and the design decides where the seam lands. Glass-filled parts need the gate planned around the weld from day one. Legacy Molding reviews every hole, boss and gate location before tooling, so the seam is not a surprise at first article. Send your CAD and annual volume for a quote with DFM notes →

Sources

Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com

Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.

Have a part like this to quote?

Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.

Request a Quote

Similar Posts