Injection Molding Tolerances: What to Specify and What Tight Tolerances Cost
Last Updated: October 24, 2026
Answer Capsule: Standard injection molding tolerances hold about plus or minus 0.005 in (0.127 mm) on most dimensions. Precision molding with tight process control holds plus or minus 0.002 in (0.05 mm) or better on critical features. The result depends on resin, wall, gate and part size, so tighten only the dimensions that matter.
Your drawing says plus or minus 0.001 in on every dimension. The quote came back at double your budget, with a note asking which dimensions matter. That note is not a dodge. Injection molding tolerances are not machining tolerances.
Plastic shrinks as it cools, grows when it picks up moisture and moves with heat. A tolerance that is routine on a machined part can be costly or impossible on a molded one. Over-tolerancing raises mold cost, slows the cycle and adds scrap, and buys nothing on dimensions that never mattered.
This post lays out what injection molding tolerances a production molder can hold and why plastic moves. It shows how resin family changes the answer, what tight tolerances cost, and how to call out only the critical dimensions. It closes with what Legacy Molding measures on the first article. The figures are the ones Brent Hanke quotes from, and they are ranges on purpose.
What are standard injection molding tolerances?
Standard, or commercial, injection molding tolerances are about plus or minus 0.005 in (0.127 mm) on a typical dimension. Precision molding holds plus or minus 0.002 in (0.05 mm) or better on critical features with tight process control. Those are the figures Legacy Molding publishes. The exact number moves with the size of the dimension, the resin, the wall and the gate.
The international reference is ISO 20457. It sets general tolerances for plastic molded parts, the limits of what a molding process can hold, and acceptance conditions. It replaced the German DIN 16742 and was revised in 2026. Its useful idea is tolerance groups. A packaging part, a housing and a precision gear sit in different groups, and you are expected to pick one.
Two practical rules follow:
- Treat plus or minus 0.005 in as the default on dimensions you do not call out as critical.
- Reserve plus or minus 0.002 in, or tighter, for the few features that locate, seal or mate.
Why can’t molded plastic hold machined-metal tolerances?
Molded plastic cannot hold machined-metal tolerances because the part changes size after it leaves the mold. The change is not perfectly repeatable. Three things move it.
Shrink. Every resin shrinks as it cools, and the mold is cut oversize to compensate. Shrink varies with wall thickness, pack pressure, mold temperature, gate location and flow direction. ASTM D955 is the test behind the shrink figure on a datasheet.
Moisture. Nylon is the usual offender. BASF’s datasheet for Ultramid A3K, a general purpose nylon 66, lists moisture pickup of 2.5 to 3.1 percent at 23 degrees C and 50 percent humidity. A nylon part grows as it conditions. Its tensile modulus on the same sheet drops from 3,000 MPa dry to 1,100 MPa conditioned.
Temperature. Plastics expand several times more than steel or aluminum per degree. A part checked at 68 degrees F in the lab is a different size on a 100 degree F assembly floor.
Callout: A plastic part is never a one to one copy of the CAD model. The mold is cut to a predicted shrink. The first article shows how close the prediction was, and the tool is tuned from there. Build that loop into your schedule.
Which materials hold tighter tolerances?
Amorphous resins hold tighter tolerances than semi-crystalline resins, because they shrink less and more evenly. ABS, PC and PC/ABS do not crystallize as they cool, so their shrink is low and nearly the same in every direction. PP, nylon, HDPE and acetal crystallize as they cool, which adds shrink and makes it sensitive to cooling rate and flow direction.
| Resin family | Structure | Datasheet shrink example | Tolerance outlook |
|---|---|---|---|
| Polycarbonate (Makrolon 2405) | Amorphous | 0.65 percent parallel, 0.70 percent normal | Tight; low and even shrink |
| ABS, PC/ABS | Amorphous | Under 1 percent on most grades | Tight; stable, little moisture effect |
| Nylon 66 (Ultramid A3K) | Semi-crystalline | 1.5 percent parallel, 1.8 percent normal | Moderate; add moisture growth |
| Polypropylene, HDPE | Semi-crystalline | Often 1 to 2.5 percent, grade dependent | Loose; high and variable shrink |
| Acetal (POM) | Semi-crystalline | Around 2 percent, grade dependent | Moderate; stable once conditioned |
| Glass-filled grades | Either, with fiber | Lower in flow, higher across flow | Tight in flow direction, warp risk |
The polycarbonate figures come from Covestro’s Makrolon 2405 datasheet.
Glass fiber cuts shrink but adds direction. A 30 percent glass-filled nylon shrinks far less along the flow than across it. That tightens one dimension and can warp a flat part. Check both shrink values on the datasheet and tell your molder which dimensions sit across the flow. The families Legacy Molding runs are on the injection molding materials page.
What do tight tolerances cost?
Tight tolerances cost money in four places: the tool, the cycle, the inspection and the scrap. None of them show up as a line called “tolerance” on the quote. That is why two quotes for the same part can differ so much.
- Tool steel and cavity count. A plus or minus 0.002 in feature usually means a hardened cavity and more polishing time. It often means fewer cavities too, because each cavity shrinks a little differently. Fewer cavities means a higher price per part.
- Cycle time. A tight dimension often needs a longer pack and cool phase and a narrower process window. A longer cycle costs more on every part for the life of the program.
- Inspection. Each critical dimension is measured on the first article and checked in-process. More critical dimensions means more measuring time per lot.
- Scrap. A tolerance at the edge of what the resin can do produces more rejects. You pay for them in the piece price.
The cheapest tolerance is the one you do not specify. A part at plus or minus 0.005 in with three critical dimensions at plus or minus 0.002 in quotes lower and runs cleaner than the same part at plus or minus 0.002 in everywhere. A realistic drawing is what keeps Legacy Molding’s 2 to 6 week production schedule.
How do you call out only the critical dimensions?
Call out only the critical dimensions by starting from function. List the features that locate, seal, mate or carry load, tolerance those, and let a general note cover the rest. Most parts have three to six dimensions that truly matter.
- Write a general tolerance note. “Unless otherwise specified, plus or minus 0.005 in” covers the bulk of the part and tells the molder the default.
- Flag critical dimensions on the drawing. Box them or list them in a table so the first article report can call them out by number.
- Tolerance from a datum the mold can hold. Dimensions across the parting line or a slide include the mold’s own variation. Dimensions inside one piece of steel are easier to hold.
- Keep walls uniform around critical features. Sink and warp live next to thick sections. The rules are in Injection Molding Wall Thickness, Ribs and Bosses: The Design Rules.
- Say which dimensions can be tuned in steel. A hole or a post is easy to open up after the first article. A cavity wall is not. Design “steel safe” where you can.
The rules on draft, walls and features that affect dimensions are in the Legacy Molding injection molding design guide.
What Legacy Molding measures on the first article
Here is a conversation Legacy Molding has most months. A quality manager sends a drawing with 40 toleranced dimensions and asks for a first article report on each one, per cavity. The tool is a transferred four-cavity mold from a supplier that went quiet. The last lot had fit problems nobody could explain.
The first step is to sort the 40 dimensions. Five matter for fit, ten affect appearance, and a general tolerance covers the rest. Legacy Molding then samples the tool with a scientific molding setup and lets the parts stabilize. Each critical dimension is measured on each cavity with calipers and height gauges, recorded by cavity number with the instrument used.
The report goes out with the resin supplier’s material cert and the lot number. On a transferred tool it usually finds the real problem: one cavity worn or shimmed differently from the other three. That is a tool fix, not a process fix. It is cheaper to find on a first article than in a rejected lot.
What the report contains is covered in First Article Inspection for Injection Molded Parts.
Frequently Asked Questions
What tolerance can injection molding hold?
Standard injection molding holds about plus or minus 0.005 in (0.127 mm). Precision molding with tight process control holds plus or minus 0.002 in (0.05 mm) or better on critical dimensions. ABS and PC hold the tight end more easily than nylon or PP.
Is plus or minus 0.001 in possible on a molded plastic part?
Sometimes, on a small feature in a low-shrink amorphous resin, in a hardened tool with few cavities. It is not realistic across a whole part, so ask your molder to review the specific feature first.
Do injection molding tolerances apply to every dimension?
No. Apply a general tolerance, usually plus or minus 0.005 in, to the whole part. Call out tighter tolerances only on the three to six dimensions that locate, seal or mate. Every extra tight dimension adds tool cost, cycle time and inspection time.
What is ISO 20457?
ISO 20457 is the international standard for tolerances and acceptance conditions on plastic molded parts. It uses tolerance groups, so a housing and a precision gear are not held to the same number. It replaced DIN 16742.
Conclusion
Plan on plus or minus 0.005 in as the standard injection molding tolerance. Reserve plus or minus 0.002 in for the few features that locate, seal or mate. Expect ABS and PC to hold tight dimensions more easily than nylon, PP or acetal. A drawing built that way quotes lower and runs faster.
Legacy Molding reviews every drawing for manufacturability before tooling. Every new or transferred tool ships with a first article report and material certs. Send your CAD and annual volume for a quote with DFM notes, or call Brent at 480-256-9773.
Sources
- ISO 20457, Plastics moulded parts, Tolerances and acceptance conditions, https://www.iso.org/standard/90304.html
- Covestro, Makrolon 2405 technical datasheet, https://solutions.covestro.com/en/products/makrolon/makrolon-2405_00945088-00009643
- BASF, Ultramid A3K product data sheet, https://download.basf.com/p1/8a8082587fd4b608017fd64108ab6d3b/en/ULTRAMID_A3K_Product_Data_Sheet_Asia_PacificEurope_English.pdf
Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com
Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.
Have a part like this to quote?
Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.