Splay in Injection Molding: Silver Streaks, Causes and Fixes
Last Updated: October 21, 2026
Answer Capsule: Splay in injection molding is silver or white streaking that fans out from the gate in the flow direction. Moisture is the usual cause: nylon, polycarbonate, ABS and PET absorb water that flashes to steam in the barrel. Heat, shear and trapped air cause the rest. Dry to the resin maker’s spec and verify with a moisture analyzer.
A lot of polycarbonate housings arrives with silver streaks fanning out from every gate, and the molder says “we dried the material.” Splay in injection molding is the defect most often blamed on the wrong thing, because moisture, heat, shear and air all leave a similar mark.
The stakes are more than cosmetic. On nylon, polycarbonate and PET, the moisture that streaks the surface also breaks polymer chains in the barrel. A part that shows splay may be weaker than its data sheet says.
This post shows you what splay looks like, where its causes live, the order a molder works the fixes, the drying numbers from the resin makers, and what to ask your molder.
What does splay look like, and how is it different from flow lines and burn marks?
Splay is a set of silver, white or dull streaks that start at the gate and spread out in the direction of flow. Moisture streaks are usually long and parabolic, with the point of each streak facing the flow direction.
The look-alikes:
- Flow lines are wavy rings or tone changes in the part’s own color that follow a slowdown in the melt. No silver.
- Burn marks are brown or black and sit at the end of fill, where trapped air scorched the plastic.
- Charred streaks from degraded melt run light brown to dark.
Color and location are the first clues. Silver at the gate says moisture, shear or air. Brown says heat. A streak in the resin’s own color at a wall change says flow.
What causes splay in injection molding?
Splay happens when gas is in the melt as it enters the cavity and breaks out at the surface as the skin freezes. Legacy Molding sorts the sources into material, process, tool and design.
| Bucket | Causes of splay |
|---|---|
| Material | Wet resin; resin dried on a schedule but never measured; wet regrind; a hopper left open overnight; over-dried resin |
| Process | Melt too hot or residence time too long; screw speed or back pressure too high; fast fill through a small gate; fast screw decompression pulling in air |
| Tool | Gate too small for the flow rate; sharp runner corners; water leaking into the cavity; nozzle tip and sprue bushing mismatch |
| Part design | A thin wall fed by a pin gate that forces high shear; no vent where the gas could escape |
Moisture leads the list. Michael Sepe, writing in Plastics Technology, notes that moisture as low as 0.07 percent can cause splay on some resins. Nylon, polycarbonate, ABS, PET and PBT also lose strength to moisture, and he puts their processing limit near 0.02 percent.
Air is the cause that fools people. John Bozzelli describes how a small gap between the nozzle tip and the sprue bushing creates a venturi effect that pulls air into the melt.
How do you fix splay, in the order a molder tries it?
You fix splay by measuring the moisture first, because it is the most common cause and the cheapest to confirm. A moisture analyzer reading beats a dryer log every time.
Here is the order Legacy Molding works through:
- Measure the resin moisture at the throat. If it is high, check dryer temperature, dew point, residence time and the desiccant.
- Dry to the spec, not the schedule. Covestro calls for four hours at 250 F (120 C), a dew point below minus 20 F, and 0.02 percent moisture or less for Makrolon polycarbonate. BASF’s data sheet for a glass-filled Ultramid nylon 66 allows up to 0.15 percent moisture with an 80 C dryer. Every grade has its own number.
- Lower melt temperature and shorten residence time. Brown-tinged streaks or a smell mean the melt is degrading.
- Slow the fill past the gate, and lower screw speed and back pressure. Shear splay fades as the melt stops tearing through the gate.
- Slow screw decompression. A fast suck-back pulls air into the front of the screw.
- Check the tool. Pressure paper on the nozzle seat, and a leak check on every water fitting.
Callout: A drying log tells you what the dryer was set to. A moisture reading tells you what the resin was. Only one of those belongs in a corrective action.
When does splay need a tool change?
Splay needs a tool change when the gate, the runner or the nozzle seat is making gas that no setting can remove. The usual repairs are opening a small gate, radiusing sharp runner corners, remachining a mismatched nozzle seat, and fixing a water line that weeps into the cavity.
The design side is smaller for splay, but it exists. A thin wall fed through a pin gate forces high shear at the gate. Brent Hanke checks gate size and location against the wall and the resin in the DFM review at Legacy Molding.
Design rules:
- Size the gate to the wall so the melt enters as a front, not a jet.
- Radius runner turns and vent at the end of fill.
- Put the resin’s moisture limit and drying conditions on the drawing or the PO, so they are a requirement, not a habit.
- When the application allows, pick a low-absorption resin. The materials Legacy Molding runs include polypropylene and HDPE, which absorb very little water. The material selection guide walks through the trade-offs.
What should you ask your molder when a lot shows splay?
Ask for the moisture reading before the lot ran, and ask who took it.
Here is a call Legacy Molding gets most months. A buyer has a lot of nylon brackets rejected for silver streaks, and the previous molder blamed the resin lot. When the tool arrives in Phoenix, Legacy Molding measures the moisture on the same resin lot. It is well above the limit.
The previous shop’s dryer was set to the right temperature with a saturated desiccant bed. The log looked fine and the resin was wet. Dry the resin to a measured value, run a first article, and the streaks are gone.
The questions to ask:
- What was the measured moisture at the throat before the lot ran, and what instrument measured it?
- What are the dryer temperature, dew point and residence time, and when was the desiccant checked?
- What was the melt temperature, and how long does a pellet sit in the barrel at this cycle?
- Is the fix a material, process or tool change, and who pays?
A corrective action note for splay should give the measured moisture before and after, the drying conditions and the melt temperature. It should also give the test that ruled air and shear in or out, and the sample that proves the fix. The other nine defects are in Injection Molding Defects: 10 Common Causes and Fixes.
Frequently Asked Questions
What causes silver streaks in injection molding?
Silver streaks, called splay, come from gas in the melt breaking out at the part surface. Moisture in the resin is the most common source, followed by heat degradation, high shear at a small gate, and air pulled in through screw decompression or a nozzle mismatch. Measure moisture first.
Which plastics are most prone to splay?
Nylon, polycarbonate, PET, PBT and ABS absorb water from the air and need drying before molding. Nylon absorbs the most. Polypropylene and polyethylene absorb very little and rarely show moisture splay.
How dry does resin need to be to avoid splay?
It depends on the resin and the grade. Covestro specifies 0.02 percent or less for Makrolon polycarbonate, and BASF’s data sheet for a glass-filled Ultramid nylon 66 allows up to 0.15 percent. Use the resin maker’s number and measure it.
Conclusion
Splay is gas in the melt, and moisture is the gas you check first. Measure it, dry to the resin maker’s number, then work through heat, shear and air in that order. A corrective action without a moisture reading is a guess.
Legacy Molding dries to a measured value, runs a scientific molding setup and ships a first article report with every new or transferred tool. Send your CAD and annual volume for a quote with DFM notes, or call Brent at 480-256-9773 with a streaked part in hand.
Sources
- Plastics Technology, Why (and What) You Need to Dry (Michael Sepe), https://www.ptonline.com/articles/why-and-what-you-need-to-dry
- Plastics Technology, The Trouble with Mismatched Nozzle Tips and Sprue Bushings (John Bozzelli), https://www.ptonline.com/articles/injection-molding-the-trouble-with-mismatched-nozzle-tips-sprue-bushings
- Covestro, Processing Information for Makrolon Polycarbonate (COV-206), https://solutions.covestro.com/-/media/covestro/solution-center/brochures/pdf/cov-206_processing-information-for-automotive-lens.pdf
- BASF, Ultramid A 218G V33 technical data sheet, https://download.basf.com/p1/8a80812f8b13e689018b3cdc23726d1d/en/Ultramid%25C2%25AE_A_218G_V33_BLACK_41N
Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com
Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.
Have a part like this to quote?
Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.