Jetting in Injection Molding: Causes, Fixes and Gate Rules
Last Updated: October 26, 2026
Answer Capsule: Jetting in injection molding is a snake-like, rough strand frozen into the surface near the gate. It happens when melt squirts through a small gate into open cavity space instead of spreading against a wall. Slow the first stage of fill, then fix the gate: larger, rounded, and aimed at a wall, core or pin.
A wormy, dull squiggle runs from the gate across the face of your clear lens, and every cavity shows it. That mark is jetting in injection molding, and it is one of the few defects that points straight at the gate. The strand shot across the empty cavity, skinned over, and got buried by the fill without fusing to it.
Jetting is a cosmetic reject on any show surface. It is also a weak spot, because the cold strand does not bond well to the melt that follows.
This post covers how to tell jetting from its look-alikes, why it happens, the fixes in order, and the gate rules that prevent it. The guidance follows the BASF troubleshooting guide and Jim Fattori’s work in Plastics Technology. The fix order is how Brent Hanke works a jetting problem at Legacy Molding in Phoenix.
What does jetting look like, and how is it different from a flow line or a weld line?
Jetting is a single rope-like strand that starts at the gate and wanders across the surface. It is often rough or dull and sometimes folded back on itself. BASF’s troubleshooting guide describes it the same way: a snake-like, often rough or matt strand starting from the gate.
The look-alikes:
- Flow lines are sets of ripples around the gate or at a wall change, running across the flow.
- Weld lines are straight seams downstream of a hole, boss or pin, nowhere near the gate.
- Splay is silver streaking that follows the flow and changes shot to shot.
What causes jetting in injection molding?
Jetting happens when the melt leaves the gate fast and meets nothing to slow it down. It shoots across the open cavity as a jet instead of spreading as a front. The jet skins over, and the melt that follows cannot fuse to the cold strand.
Jim Fattori makes the point plainly in Plastics Technology. No matter the gate type, “unless the material is crawling into the cavity, they all jet to some degree until they hit an obstruction.” The distance from the gate to the first obstruction usually decides it.
| Bucket | What causes or worsens jetting |
|---|---|
| Material | Low-viscosity grades, melt run cold so the strand skins fast |
| Process | High injection speed through the gate, low melt temperature, low mold temperature, no first-stage speed profile |
| Tool | Small gate, sharp gate-to-part transition, gate aimed into open space, steep tunnel gate angle |
| Design | Thick open cavity right at the gate, no wall or core pin for the melt to strike |
How do you fix jetting, in order?
Start with the speed profile, then temperature, then the gate.
- Slow the first stage of fill. Program a slow speed until the melt clears the gate and touches a wall, then ramp up. It costs nothing and works most often.
- Raise melt temperature inside the resin maker’s window. BASF pairs it with reduced injection speed.
- Raise mold temperature so a strand, if it forms, stays soft long enough to fuse.
- Enlarge the gate. Fattori’s example: a 0.030 inch gate will jet more into a 0.100 inch wide cavity than a 0.060 inch gate will.
- Radius the gate-to-part transition. BASF lists rounding this transition as a fix.
- Move or change the gate so the melt strikes an obstacle at once: a cavity wall, a core pin, an ejector pin or a rib.
Steps 1 to 3 belong to the first sampling session. Steps 4 to 6 are tool work.
Which gate designs stop jetting?
A gate that lands the melt on steel stops jetting, and a gate that fires into open space causes it. The type matters less than where it points.
| Gate | Jetting risk | Why |
|---|---|---|
| Pin or tunnel gate into an open flat face | High | Small cross section, melt fires into free space; a steeper tunnel angle makes it worse |
| Edge gate aimed at the opposite wall or a core pin | Low | Melt strikes steel right away and spreads as a front |
| Fan gate | Low | Wide, thin entry slows the melt and spreads it before it enters |
| Tab gate | Low | Melt enters a small tab first, loses speed, then flows into the part |
| Overlap gate | Low | Gate lands on the part face, so the melt hits the cavity wall as it enters |
Design rules that prevent jetting
Here is a call Legacy Molding gets most months. A buyer has a clear polycarbonate lens the size of a coin, pin-gated at the center of the domed face. Every part has a worm from the center to the rim. Slowing the fill and raising melt temperature faded it but never cleared it.
The fix was a tool change. A sub gate on the back rim, aimed at the inside wall of the dome, made the melt hit steel at once and spread. The dome came out clear, and the gate vestige moved to a hidden face.
Rules that keep jetting off your drawing:
- Put the gate where the melt hits a wall, core or pin first. Gate off an edge into the side wall, or onto the inside of a boss.
- Keep the gate out of the middle of a show surface. If a center gate is unavoidable, plan a fan or tab gate.
- Round the gate-to-part transition in the model.
- Name the cosmetic surface on the drawing, so the gate location is a design decision, not a tooling convenience.
The injection molding design guide covers gate location with the wall and draft rules Legacy Molding checks in DFM review. The injection molding defects hub shows how jetting relates to the other nine common defects.
When does jetting need a tool change?
Jetting needs a tool change when the slow-start profile and the temperature window are used up and the strand still shows. The signs: the mark sits in the same place whatever the profile, or the gate is a pin gate in the center of an open face. Opening or radiusing a gate is a small cut; moving the gate or changing its type is bigger. Legacy Molding handles that through its tooling and mold transfer process, with a fresh first article after the change.
What to ask your molder about jetting
Ask what the first-stage speed profile looks like, what gate the tool has, and what the melt hits when it leaves the gate. A corrective-action note should state the cavity with a photo, the speed profile and temperatures before and after, and the gate size, type and location with any change. Brent Hanke keeps the setup sheet and the FAI together on every Legacy Molding tool, so the profile that cleared the jetting is the one the next run starts from.
Frequently Asked Questions
Is jetting a strength problem or just cosmetic?
Both. The strand cools before the rest of the fill arrives, so it does not fuse well. BASF’s guide notes that this leads to a poor appearance and reduced strength along the strand.
Can injection speed alone fix jetting in injection molding?
Often, yes, if the gate is near a wall. A slow first stage, then a fast fill, clears most cases. If the gate fires into open space, speed only fades it.
Does a hot runner stop jetting in injection molding?
No. A hot runner drop jets the same way a cold gate does until the melt meets an obstruction. The drop location decides it, not the runner type.
What is an overlap gate?
An overlap gate is an edge gate that lands on the face of the part instead of its edge, so the melt hits the cavity wall as it enters. It leaves a vestige on the face, so it goes on a non-cosmetic surface.
Conclusion
Jetting is melt shooting across an open cavity, so slow it down at the gate or give it steel to hit. A slow first-stage profile clears most cases for free. A larger or radiused gate clears more, and a gate aimed at a wall, core or pin prevents it for good. Legacy Molding checks gate placement against the cosmetic surfaces in DFM review on every part. Send your CAD and annual volume for a quote with DFM notes →
Sources
- BASF, Injection Molding Problems in Engineering Thermoplastics: Causes and Solutions, https://download.basf.com/p1/8a8082587fd4b608017fd6631d5a24b1/en/Injection-Molding_Problems_in_Engineering_Thermoplastics_-_Causes_and_Solutions_Brochure_English.pdf
- Plastics Technology, Tunnel Gates for Mold Designers, Part 1 (Jim Fattori), https://www.ptonline.com/articles/tooling-tunnel-gates-for-mold-designerspart-1
Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com
Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.
Have a part like this to quote?
Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.