Sink Marks in Injection Molding: Causes, Fixes, Design Rules
Last Updated: October 23, 2026
Answer Capsule: Sink marks in injection molding are shallow dimples on the surface opposite a thick section, rib or boss. The skin freezes first, then the thick core keeps shrinking and pulls the skin inward. Causes are thick walls, ribs over 50 to 60 percent of the wall, low pack pressure or time, and a gate that freezes early.
A sink mark over a screw boss on the show face of a housing is the reject incoming inspection sends back most often. Sink marks in injection molding are small, usually a few thousandths deep, and still visible from across the room on a glossy black part.
The part is complete, the dimensions are in tolerance, and the lot still fails. The cause is usually in the part design, so packing harder only hides it for a while.
This post shows you what sink marks look like, where their causes live, the order a molder works the fixes, and the rib and boss rules that prevent them.
What do sink marks look like, and how do you tell them from voids?
A sink mark is a shallow depression on an outside surface, directly opposite a rib, a boss, a wall step or any other thick section. It shows as a dull spot or a shadow under a light held at a low angle.
A void is the same shrinkage with a different result. If the skin is stiff enough to hold its shape, the shrinking core pulls away from the inside and leaves a bubble. The surface stays flat.
- Sink: surface pulled in, interior solid.
- Void: surface flat, interior hollow.
What causes sink marks in injection molding?
Sink marks happen when a thick section keeps shrinking after the surface has frozen and no more melt is coming through the gate. All plastics shrink as they cool, and mold shrinkage is measured under ASTM D955. Semi-crystalline resins such as polypropylene, nylon and acetal shrink more than amorphous resins such as ABS and polycarbonate. So they sink more at the same geometry.
| Bucket | Causes of sink marks |
|---|---|
| Material | A high-shrink resin on a thick design; regrind changing shrink |
| Process | Pack pressure too low; hold time shorter than gate seal; melt or mold too hot; cushion lost |
| Tool | Gate too small, so it freezes before pack is done; gate far from the thick section; poor cooling behind the thick area |
| Part design | Wall too thick; rib or boss wall over 50 to 60 percent of the nominal wall; boss merged into a side wall; sudden wall step |
Peter Zuber of SABIC, writing in Plastics Technology, puts the process side simply: a shorter packing phase increases shrinkage and gives more or larger sink marks. He also notes that small tunnel gates freeze early and cut the packing window short.
The design side has published ratios. Covestro’s part and mold design guide gives a rib at 50 percent of the wall for minimal sink and 66 percent for slight sink on polycarbonate and PC/ABS. It drops the rib to 40 percent for high gloss surfaces.
How do you fix sink marks, in the order a molder tries it?
You fix sink marks by packing more melt into the thick section before the gate freezes. The test for that is a gate seal study, and John Bozzelli’s Plastics Technology column on gate seal testing lays it out.
Start with a very short hold time and add time in steps. Weigh the parts and find where part weight stops climbing. That is gate freeze. Holding past it does nothing, and holding short of it leaves the thick section unpacked.
Here is the order Legacy Molding works through:
- Run a gate seal study and set hold time at or just past gate freeze.
- Raise pack pressure in steps, watching for flash on the parting line.
- Lower melt and mold temperature behind the thick section, so the core freezes sooner.
- Move the transfer position so the part is nearly full at transfer.
- Open the gate or change the gate type so it stays open long enough to pack. This is a tool change.
- Add cooling behind the thick section, or fit a more conductive insert.
Callout: Process can hide a sink. It cannot remove the thick section that causes it. If the sink comes back when the tool warms up or the resin changes, the design is the cause.
When do sink marks need a tool change or a design change?
Sink marks need a tool change when the gate freezes before the thick section is packed and no hold setting fixes it. They need a design change when the rib, boss or wall step is too thick for the resin. The design change is often a small cut on the existing steel. Examples are coring a boss base, recessing the outside face around a boss, or thinning a rib by adding steel to the cavity.
Brent Hanke checks every rib, boss and wall step against these ratios in the DFM review at Legacy Molding. The rules:
- Ribs at 50 to 60 percent of the wall, no taller than three times their base, with a small root radius.
- Bosses at the same wall ratio, cored to the base wall, stood off side walls on a thin rib, with an outside recess if they must be thicker.
The numbers by resin are in Injection Molding Wall Thickness, Ribs and Bosses: The Design Rules. The full set of feature rules is in the injection molding design guide.
What should you ask your molder when a lot sinks?
Ask whether the sink was there at first article. If it was, the design is the cause.
Here is a call Legacy Molding gets most months. A design engineer has an ABS cover with sink over four bosses, and the previous molder packed harder until the parting line flashed. When the tool arrives in Phoenix, Legacy Molding samples it as received and runs a first article.
The bosses are solid at the base and merged into the side wall. A gate seal study shows the gate freezing well before the bosses can pack. The fix is a small core pocket in each boss base and an outside recess, a modest cut on the existing tool. A second first article shows the sink gone at a lower pack pressure.
The questions to ask:
- Was the sink on the first article report, or did it appear later?
- What hold time did the gate seal study give, and what is set now?
- What are the rib and boss thicknesses as a percentage of the wall?
- Is the fix a setting, a gate change or a core pocket, and who pays?
A corrective action note for sink should give the first article comparison, the gate seal data and pack pressure before and after. It should also give the change made and the sample that proves it. The other nine defects are in Injection Molding Defects: 10 Common Causes and Fixes.
Frequently Asked Questions
What causes sink marks on plastic parts?
Sink marks come from a thick section that keeps shrinking after the surface has frozen. Ribs, bosses and wall steps cool slower than the wall around them, and as their core shrinks it pulls the skin inward.
How thick can a rib be without sink marks?
Keep a rib at 50 to 60 percent of the wall it sits on. Covestro’s design guide puts minimal sink at 50 percent and slight sink at 66 percent for polycarbonate and PC/ABS. It drops to 40 percent for high gloss surfaces. Filled grades tolerate a thicker rib because they shrink less.
Can you fix sink marks by increasing pack pressure?
Only until the gate freezes. Run a gate seal study first, because pack pressure after gate freeze does nothing. If the rib or boss is too thick for the resin, the lasting fix is to thin or core the feature.
Conclusion
Sink marks come from a thick section that shrinks after the skin has set. Pack it better with a gate seal study and the right hold time. Open the gate if it freezes too soon, and fix the rib or boss ratio if the sink keeps coming back.
Legacy Molding checks every rib, boss and wall step in the DFM review, and every new or transferred tool gets a first article. Send your CAD and annual volume for a quote with DFM notes, or call Brent at 480-256-9773 with a sunk part in hand.
Sources
- ASTM D955, Standard Test Method of Measuring Shrinkage from Mold Dimensions of Thermoplastics, https://store.astm.org/d0955-21.html
- Plastics Technology, How to Reduce Sinks in Injection Molding (Peter Zuber, SABIC), https://www.ptonline.com/articles/how-to-reduce-sinks
- Covestro, Engineering Polymers: Part and Mold Design, Thermoplastics, A Design Guide, https://solutions.covestro.com/-/media/covestro/solution-center/brands/downloads/imported/1557214249.pdf
- Plastics Technology, Gate-Seal Testing Done Right (John Bozzelli), https://www.ptonline.com/articles/injection-molding-gate-seal-testing-done-right-
Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com
Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.