Short Shots in Injection Molding: Causes and Fixes
Last Updated: October 22, 2026
Answer Capsule: A short shot in injection molding is a part that did not fill: a missing corner or an unfilled rib at the end of the flow path. Causes are too little shot, low fill speed or pressure, cold melt or mold, trapped air with no vent, small gates, or a wall too thin for its flow length.
A lot comes back with the last rib on every housing missing, and the molder says the press “needed more pressure.” A short shot in injection molding is the most basic defect there is, and still one of the easiest to misdiagnose. Pressure is the fix people reach for, and the cause is often somewhere else.
A short shot also points at one of the oldest design limits in molding: how far a resin can flow through a wall before it freezes.
This post shows you what a short shot looks like, where its causes live, the order a molder works the fixes, the flow length rule that prevents it, and what to ask your molder.
What does a short shot look like, and what else looks like it?
A short shot is a part with material missing at the last place the melt reached. That is usually a corner far from the gate, the tip of a thin rib, or a thin window between thick sections. The edge of the missing area is rounded and glossy, because the flow front stopped and froze.
Look-alikes:
- A burn mark at the same spot. Trapped air can scorch the plastic before the cavity shorts. A short with a brown edge is a venting problem.
- A cold slug. A cold slug can block a gate and short one cavity while the others fill.
Where and when the short happens narrows the cause. A short on every cavity in the same place is process or design. A short on one cavity is a gate, a vent or a runner for that cavity. A short that comes and goes shot to shot is a shot size or check ring problem at the press.
What causes a short shot in injection molding?
A short shot happens when the melt freezes before the end of the cavity, or when something stops it getting there. Legacy Molding sorts the causes into material, process, tool and part design.
| Bucket | Causes of short shots |
|---|---|
| Material | Lower flow grade than the tool was cut for; a lot with a different melt flow rate; too much regrind; wet resin |
| Process | Shot size too small; transfer too early; fill too slow; melt or mold too cold; worn check ring losing cushion |
| Tool | Vents blocked or too shallow; gate or runner too small; unbalanced runner; no cold slug well; blocked nozzle or hot runner drop |
| Part design | Wall too thin for the flow length; a thin window between thick sections; a tall thin rib at the end of fill |
Venting is the cause most often skipped. Suhas Kulkarni’s vent depth study in Plastics Technology lists what happens when vents are too shallow: short shots, poorly packed parts, burning, voids and dimensional variation.
Flow length is the design cause. Every resin has a limit on how far it flows through a given wall before the skin freezes. Covestro’s design guide treats walls under about 1.5 mm as thin-wall molding that may need higher pressure and a high flow grade.
How do you fix a short shot, in the order a molder tries it?
You fix a short shot by finding where the melt stops and why, and the tool for that is a deliberate short shot. John Bozzelli’s Plastics Technology column on making a short shot on purpose describes the method. Drop second-stage pressure to the minimum and watch the fill pattern grow shot by shot. The last place to fill is where the vent belongs.
Here is the order Legacy Molding works through:
- Confirm the cushion and the transfer position. A press that bottoms out has nothing left to pack.
- Raise shot size and fill speed before raising pressure.
- Raise melt and mold temperature inside the resin maker’s window.
- Clean the vents and check their depth. Fix a burned edge here, before touching pressure.
- Open the gate or balance the runner if one cavity shorts and the others fill.
- Change to a higher flow grade of the same resin family if the wall and flow length will not move.
Callout: Pressure is the last lever, not the first. A short fixed with pressure alone usually comes back as flash, a crushed vent or a stressed part.
When does a short shot need a tool change?
A short shot needs a tool change when the melt stops in the same place at every setting inside the resin window. The usual repairs are adding or deepening vents at the last place to fill, or opening a gate or runner branch. Others are adding a flow leader or moving the gate toward the far end of the part. A flow leader is a slightly thicker channel that feeds a thin area.
Brent Hanke checks flow length against wall thickness and gate location in the DFM review at Legacy Molding. A thin far corner is obvious in CAD and expensive in a hardened tool. The rules:
- Keep the wall uniform and above the resin’s thin-wall limit, usually 1 mm or more on small parts.
- Gate into the thick section so the melt flows thick to thin.
- Add a flow leader or a second gate for a thin area far from the gate.
Wall ranges by resin are in Injection Molding Wall Thickness, Ribs and Bosses: The Design Rules. The full set of feature rules is in the injection molding design guide.
What should you ask your molder when a lot comes up short?
Ask to see the short-shot study. If the molder cannot show you the fill pattern, nobody knows where the melt stops.
Here is a call Legacy Molding gets most months. A founder has a polycarbonate enclosure that shorts at one far corner every few shots. The previous molder has been raising pressure for a month. When the tool arrives in Phoenix, Legacy Molding samples the tool and runs a progressive short-shot study.
The corner is the last place to fill and there is no vent near it. The setup sheet shows the cushion wandering because the check ring is worn. A new check ring, a vent at the corner and a lower pack pressure fix it. A first article confirms the fill is stable.
The questions to ask:
- Where is the last place to fill, and is there a vent there?
- Is the cushion holding shot to shot, and when was the check ring last checked?
- Which cavities short, and are the runners balanced?
- Is the fix a setting, a vent, a gate or a wall change, and who pays?
A corrective action note for a short shot should show the fill pattern, the cushion data and the vent depths measured. It should also show the change made and the sample that proves it. The other nine defects are in Injection Molding Defects: 10 Common Causes and Fixes.
Frequently Asked Questions
What is a short shot in injection molding?
A short shot is a molded part that did not fill completely. The melt froze or ran out of pressure before it reached the end of the cavity. The result is a missing corner, rib or edge with a rounded, glossy boundary.
Why does only one cavity short on a multi-cavity mold?
One cavity shorting while the others fill points at that cavity, not the press. The usual causes are a blocked or shallow vent, a smaller gate, an unbalanced runner branch, or a cold slug blocking the gate.
Does raising injection pressure fix short shots?
Sometimes, but it should be the last change, not the first. Shot size, fill speed, temperature and venting fix most short shots without more pressure.
Conclusion
A short shot means the melt stopped before the end of the cavity. Find where it stops with a short-shot study. Fix the cushion, speed, temperature and venting in that order, and treat pressure as the last lever.
Legacy Molding checks flow length and gate location in the DFM review, and every new or transferred tool gets a first article. Send your CAD and annual volume for a quote with DFM notes, or call Brent at 480-256-9773 with a short part in hand.
Sources
- Plastics Technology, Determining Vent Depths in Injection Molding (Suhas Kulkarni), https://www.ptonline.com/articles/determining-vent-depths-in-injection-molding
- Plastics Technology, Good Reasons to Make a Short Shot, and How to Do It Right (John Bozzelli), https://www.ptonline.com/articles/good-reasons-to-make-a-short-shot-and-how-to-do-it-right
- Covestro, Engineering Polymers: Part and Mold Design, Thermoplastics, A Design Guide, https://solutions.covestro.com/-/media/covestro/solution-center/brands/downloads/imported/1557214249.pdf
Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com
Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.
Have a part like this to quote?
Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.