Injection Molding Defects: 10 Common Causes and Fixes

Last Updated: October 22, 2026

Answer Capsule: Injection molding defects come from four sources: the material (moisture, regrind), the process (temperature, pressure, speed, cooling), the tool (venting, gates, cooling layout, wear) and the part design (walls, ribs, draft). The ten most common are short shots, flash, sink marks, warp, weld lines, splay, burn marks, jetting, flow lines and voids. Each has a known cause and fix.

A lot just failed inspection and the molder’s answer was “we adjusted the process.” That is not an answer. Injection molding defects cost you a scrapped run, a late ship date or a field failure. You cannot sign off on a corrective action you do not understand.

Most molded-part defects are not mysteries. Each one leaves a signature on the part. A silver streak fanning out from the gate says one thing, and a dimple opposite a rib says another. Read the signature and you can trace it to the material, the process, the tool or the design.

This guide covers the ten injection molding defects Legacy Molding sees most often, with the cause and fix for each. It adds a troubleshooting table and the questions to ask when a lot fails.

What causes injection molding defects?

Almost every injection molding defect traces back to one of four sources: the material, the process, the tool or the part design. The buckets matter because the fix lives in a different place for each. A process fix takes an hour, a tool fix takes a trip to the tool room, and a design fix takes a new revision before you cut steel.

  • Material. Wet resin, too much regrind, a lot that changed, or the wrong grade for the flow length.
  • Process. Melt and mold temperature, fill speed, pack pressure, hold time, cooling time, transfer point.
  • Tool. Vents, gate size and location, cooling layout, worn parting lines, damaged cores and pins.
  • Design. Uneven walls, thick ribs, uncored bosses, sharp corners, no draft, long thin flow paths.

One defect can have causes in more than one bucket. A sink mark can be a thick rib (design), a gate that freezes early (tool) or low pack pressure (process). Brent Hanke at Legacy Molding runs a DFM review on every part before tooling because design causes are the cheapest to fix and the most expensive to ignore.

The 10 most common injection molding defects, with causes and fixes

Here are the ten defects you will see most often, with fixes listed cheapest first.

1. Short shots

A short shot is a part that did not fill. You see a missing corner, an unfilled rib or a thin area that stopped before the end of the flow path.

Causes: Too little material in the shot, low injection pressure or speed, melt or mold too cold, trapped air with no vent, small gates, or a wall too thin for the flow length.

Fixes: Raise the shot size or move the transfer point. Raise melt and mold temperature within the resin maker’s window. Fill faster. Clean or add vents at the last place to fill. Open the gate or add a flow leader.

2. Flash

Flash is a thin skin of plastic where there should be none: along the parting line, around ejector pins or in the vents.

Causes: Clamp tonnage too low for the projected area, a worn parting line, overpacking from too much pressure or a late transfer, melt too hot and thin, or debris on the parting surface. Flash that creeps in over months is tool wear. Flash that appears today is process.

Fixes: Check tonnage against projected area. Lower pack pressure and transfer earlier. Lower melt temperature. A worn parting line needs a refit, not a retune.

3. Sink marks

Sink marks are shallow dimples opposite a thick section, a rib or a boss. The outside skin freezes first, then the thick core keeps shrinking and pulls the skin inward.

Causes: Thick walls, ribs thicker than about 50 to 60 percent of the wall, a gate that freezes before pack finishes, too little pack pressure or hold time, or a mold running hot in that zone. Mold shrinkage is tested under ASTM D955, and high-shrink resins like polypropylene and nylon sink more than ABS or polycarbonate.

Fixes: Raise pack pressure and extend hold until the gate seals. Open the gate. The lasting fix is design: thin the rib to 50 to 60 percent of the wall and core out the boss. See the wall thickness, rib and boss rules for the numbers.

4. Warp

Warp is a part that twists, bows or cups after ejection. Flat parts, long parts and glass-filled parts warp the most.

Causes: Uneven cooling between the mold halves, walls that shrink at different rates, fiber orientation in glass-filled resins, or ejecting while the part is still soft. Semi-crystalline resins (polypropylene, nylon, acetal) shrink more than amorphous resins (ABS, polycarbonate), so they warp more.

Fixes: Balance cooling so both halves run close in temperature. Extend cooling time. Make the walls uniform. Move the gate so flow runs one direction across the part. A warped part that must be flat is often a resin change, not a process change.

5. Weld lines and knit lines

A weld line is the seam where two flow fronts meet. You see it past a hole, a core pin or a boss, and wherever two gates feed one cavity. It is cosmetic on some parts and a weak point on others.

Causes: The fronts arrive cold and do not fuse: low melt or mold temperature, slow fill, trapped air at the seam, or mold release on the steel. Glass-filled resins show weak weld lines because fibers do not cross the seam.

Fixes: Raise melt and mold temperature. Fill faster so the fronts meet hot. Vent at the weld. Move the gate so the weld lands where it carries no load and does not show.

6. Splay and silver streaks

Splay shows as silver or white streaks that fan out from the gate in the flow direction.

Causes: Moisture first. Nylon, polycarbonate, ABS and PET absorb water, and water flashes to steam in the barrel. The other causes are heat (melt too hot, residence too long) and shear (melt forced through a small gate too fast).

Fixes: Dry to the datasheet time and temperature, and verify with a moisture analyzer rather than a drying log. Lower melt temperature and shorten residence time. Slow the fill past the gate. Ask for the material cert and the dryer record on any splay reject.

7. Burn marks

Burn marks are brown or black marks at the end of fill, at the bottom of a deep rib or in a blind pocket.

Causes: Trapped air. When the melt compresses air that cannot escape, the air heats enough to scorch the plastic, the “diesel effect.” Fast fill, blocked vents and hot melt make it worse.

Fixes: Clean the vents. Add vents at the last place to fill. Slow the end of the fill profile. Lower melt temperature. Burns that return after every cleaning are a tool venting problem.

8. Jetting

Jetting looks like a snake frozen into the surface near the gate. The melt shot across the open cavity as a thin stream and froze before the rest of the fill buried it.

Causes: The melt enters open space without touching a wall, because the gate points into the cavity, the gate is small, the fill is fast or the mold is cold.

Fixes: Slow the first stage of fill so the melt enters as a front. Open the gate. Raise mold temperature. The lasting fix is a gate aimed at a wall or core, such as a fan gate or tab gate.

9. Flow lines

Flow lines are wavy rings, streaks or tone changes on the surface, usually near the gate or at a wall change.

Causes: The melt cools as it flows and the surface records every slowdown. Low mold temperature, slow fill, sharp corners, sudden wall changes and a gate placed where flow stalls.

Fixes: Raise mold temperature. Fill faster. Round the corners and blend wall transitions. Gate into a thick section so the melt flows thick to thin. A deeper texture hides lines a polished surface shows.

10. Voids

Voids are bubbles trapped inside thick sections. You find them when a part cracks, fails a leak test or gets cut open. Plastics Technology covers the pack and hold fixes for voids and sinks in detail.

Causes: The skin freezes and the thick core shrinks away from it, leaving a vacuum pocket. Thick walls, early gate freeze, low pack pressure or a fast fill that traps gas. Moisture can also leave gas bubbles, which look different in a cut section.

Fixes: Slow the fill. Raise pack pressure and hold time. Open the gate so it stays unfrozen longer. As with sink, the real fix is design: thin the section and add ribs for stiffness instead of mass.

Rule of thumb: A defect at the gate points to speed and gate size. A defect at the end of fill points to venting and temperature. A defect opposite a thick section points to design.

Injection molding defects troubleshooting table

Use this table to narrow a defect to its likely bucket before you call the molder. The bucket names match the four sources above.

Defect Most likely bucket First fix Lasting fix
Short shot Process, then tool Raise shot size, speed, temperature Vent, open gate, thicken wall
Flash Process, then tool wear Lower pack pressure, check tonnage Refit parting line
Sink marks Design, then process Raise pack and hold Thin rib to 50 to 60 percent of wall
Warp Tool cooling and design Balance cooling, longer cool time Uniform walls, gate location, resin
Weld lines Process, then tool Raise melt and mold temperature Vent at weld, move gate
Splay Material Dry resin, verify moisture Lower melt temp, open gate
Burn marks Tool venting Clean vents, slow end of fill Add vents
Jetting Tool gate Slow first stage of fill Gate into a wall
Flow lines Process, then design Raise mold temp, fill faster Round corners, blend walls
Voids Design, then process Raise pack, slow fill Thin section, core out

How do you find the root cause when a lot fails?

You find root cause by changing one thing at a time and checking whether the defect follows the material, the setting, the cavity or the design. The first question is simple: what changed since the last good lot?

Here is a call Legacy Molding gets most months. A buyer has a lot of polycarbonate housings rejected for silver streaks, and the previous molder “tweaked the temperature” with no result. When the tool arrives in Phoenix, the first check is the material, and the resin turns out to have been dried on a schedule rather than to a measured moisture level. Dry it correctly, run a first article, and the streaks are gone.

Work through the buckets in this order:

  1. Material. Pull the material cert. Check drying time, temperature, the moisture reading and the regrind ratio.
  2. Process. Compare the current setup sheet to the last good one, setting by setting.
  3. Tool. Ask whether the defect appears in every cavity or one. A single bad cavity points at a vent, a gate or a damaged core.
  4. Design. If the defect has been there since the first article and gets worse with speed, the design is the cause.

A defect in one cavity is almost never a process problem. A defect in every cavity at the same spot is almost never a tool problem.

What should you ask your molder when a lot fails?

Ask for the evidence, not the explanation. A good molder can show the data behind a corrective action in a day. Legacy Molding ships a first article inspection report with every new or transferred tool, so the baseline is always on file.

  • Which cavities show the defect, and at what rate?
  • What was the measured moisture of the resin before it ran?
  • Can you send the setup sheet for this lot next to the one for the last good lot?
  • Does the defect appear on the first article report for this tool?
  • Is the fix a process change, a tool repair or a design change, and who pays?

Ask for a sectioned part if the defect is internal. The inside of a void tells you whether it was vacuum (clean and shiny) or gas (rough and pitted). One cut can end a week of back and forth.

Which defects can you fix on the drawing before tooling?

Sink marks, voids, warp and weld lines most often start on the drawing, and all four are cheaper to fix in CAD than in steel. That is why Legacy Molding reviews every part for manufacturability before quoting.

  • Keep wall thickness uniform, with tapers instead of steps.
  • Hold ribs to 50 to 60 percent of the wall and about three times the wall in height.
  • Core and gusset every boss, and radius every corner.
  • Draft every vertical face, with more on textured surfaces.
  • Place holes where a weld line can land without carrying load.

The injection molding design guide covers each rule with numbers by material. Resin choice moves the risk too. Among the materials Legacy Molding runs, the right pick for a flat cosmetic part is often the lower-shrink amorphous one.

Deeper dives on each defect

Legacy Molding publishes a short troubleshooting post on each defect, with the causes grouped by material, process, tool and design, and the fixes in the order a molder tries them.

Frequently Asked Questions

What is the most common injection molding defect?

Short shots, flash and sink marks are the most common injection molding defects in most shops, with splay close behind on nylon and polycarbonate. Short shots and flash are opposite ends of the same fill and pack balance. Sink marks are usually a design issue hiding behind a process setting.

Why do my injection molded parts have silver streaks?

Silver streaks, called splay, are almost always moisture in the resin. Nylon, polycarbonate, ABS and PET absorb water, and that water turns to steam in the barrel and streaks the surface. Dry to the resin maker’s specification and confirm with a moisture analyzer, not a drying log.

How do I know if a defect is the molder’s fault or a design problem?

Look at the first article report. A defect present on the first article that gets worse as the process speeds up is a design limit. A defect that appeared after a clean first article is a material, process or tool-wear issue on the molder’s side. Setup sheets and material certs show which.

Conclusion

Every injection molding defect comes from the material, the process, the tool or the design. The fix lives in the same bucket as the cause, and the defect’s location tells you where to look first. The molder’s job is to show you the data.

Legacy Molding reviews the design before cutting steel, runs a scientific molding setup and ships a first article report with every tool. Send your CAD and annual volume for a quote with DFM notes, or call Brent at 480-256-9773 with a failed lot in hand.

Sources

Brent Hanke | Legacy Molding | 480-256-9773 | b.hanke@legacy-molding.com

Brent Hanke is the owner of Legacy Molding, a custom plastic injection molder in Phoenix, Arizona, producing parts for OEMs across the Southwest and the country.

Have a part like this to quote?

Send the CAD and annual volume. A Phoenix engineer replies within one business day with pricing and DFM notes.